Design rules
Troubleshooting: what to change when a snap-fit fails
From the symptom to the cause and the fix: hooks that break, joints that are too stiff, rattle, loosen or cannot be released.
Hook breaks or turns white at the root while joining: the strain at the root is above the permissible strain of the material (BASF, Part III; Bayer, Table 1). A sharp corner at the root is the most common single cause; use a fillet radius of at least half the beam thickness and never less than 0.38 mm (BASF, Part VI; Bayer, p. 8). A longer or thinner beam lowers the strain; a beam tapered to half its thickness allows more than 60 % more deflection (Bayer, p. 12).
Joining force too high: the mating force grows with the deflection force and with friction and the lead angle, W = P · (μ + tan α) / (1 − μ · tan α) (BASF, Fig. III-2). A gentler lead angle, a more flexible beam or a material pair with less friction helps; two parts of the same plastic usually have higher friction than plastic on steel (Bayer, Table 3; BASF, Table IV-II).
Joint cannot be released although it should be: with μ · tan α′ at 1 or above, the joint is self-locking (BASF, Fig. III-2; Bayer, p. 14). Reduce the return angle. If it is opened often, also design with about 60 % of the one-time permissible strain (Bayer, Table 2).
Assembly rattles or has play: the tolerances of both parts add up (BASF, Part I and Part VI). A deeper overhang and a worst-case tolerance study keep the pull-off force (BASF, Part VI); check the strain at the upper limit of the undercut and the holding force at the lower limit.
Holding force drops over time or a seal starts to leak: plastics relax under constant load (BASF, Part VI). A low-stress beam, a 90° return angle, or a large return angle with a longer land in the return area keeps the joint tight (BASF, Part VI, Fig. VI-2, VI-3).
Hook fails only after many openings: fatigue. Choose a material known to perform well in fatigue and check the design stress with its S-N curves at the operating temperature (BASF, Part VI).
Nylon parts behave differently depending on the season: nylon changes with moisture, so check both the dry-as-moulded and the conditioned state (BASF, Part III).
Mould needs a slide and becomes expensive: a slot in the wall directly below the undercut or snaps on the outer edge facing outwards can avoid it; U-shaped snaps can carry the undercut on the outer edge (BASF, Part I, Fig. I-1; BASF, Part V).
Key points
- Breaks at the root: lower the strain and add a root radius.
- Too stiff: smaller lead angle, more flexible beam, less friction.
- Rattles: worst-case tolerances. Loosens: relaxation, 90° return angle.
Open the calculator Open the snap type selector
Sources
- BASF Snap-Fit Design Manual, Parts I, III, V, VI, Fig. III-2, Table IV-II
- Bayer, Snap-Fit Joints for Plastics, p. 8, 12, 14, Tables 1–3
Articles summarise the sources in our own words. They do not replace the design guides, your datasheet or tests with real parts.